Research Article
Effect of Double Transition Metal Salt Catalyst on Fushun Oil Shale Pyrolysis
Table 3
Comparison among thermogravimetric data of different samples.
| Samples | Starting temperature/°C | Termination temperature/°C | Maximum weight loss rate /%/min | Temperature at maximum weight loss rate/°C | Sample weight loss rate/wt.% | Room temperature~200°C | 200~600°C | 600~900°C |
| OS | 418.1 | 520.8 | 1.609 | 471.2 | 0.10 | 15.07 | 3.15 | OS-SA | 413.7 | 517.4 | 1.654 | 470.4 | 0.11 | 15.36 | 3.55 | OS-Cu1Ni0/SA | 396.5 | 520.2 | 1.420 | 469.0 | 0.44 | 16.12 | 3.99 | OS-Cu2Ni1/SA | 392.9 | 519.2 | 1.589 | 467.2 | 0.55 | 17.05 | 3.83 | OS-Cu1Ni1/SA | 398.0 | 520.0 | 1.517 | 467.6 | 0.20 | 16.98 | 3.47 | OS-Cu1Ni2/SA | 401.8 | 520.3 | 1.499 | 468.0 | 0.33 | 16.14 | 3.85 | OS-Cu0Ni1/SA | 394.5 | 515.7 | 1.586 | 458.3 | 0.59 | 17.35 | 4.17 |
|
|