Research Article
Microstructure and Mechanical Properties of Recycled Aggregate Concrete in Seawater Environment
Table 4
Compressive strength of RAC with seawater corrosion (MPa).
| Corrosion time (Months) | NC | RC-30 | RC-60 | Peak value | Mean value | Peak value | Mean value | Peak value | Mean value |
| 4 | 28.90 | 28.92 | 25.30 | 27.34 | 25.40 | 25.79 | 29.46 | 27.80 | 27.95 | 28.40 | 28.91 | 24.01 |
| 8 | 31.30 | 28.39 | 25.58 | 26.66 | 26.87 | 24.99 | 27.72 | 27.98 | 24.60 | 26.14 | 26.42 | 23.50 |
| 12 | 26.20 | 26.86 | 25.40 | 25.70 | 23.20 | 23.43 | 27.10 | 27.20 | 22.98 | 27.28 | 24.49 | 24.10 |
| 16 | 27.80 | 25.80 | 23.98 | 23.49 | 22.64 | 22.11 | 25.30 | 22.20 | 21.60 | 24.30 | 24.30 | 22.08 |
|
|