Composition and parameters used for production of the glass samples. M/A refer to melting/annealing.

SampleGlass composition (wt.%)Dopants (wt.%)M/A temperature (°C)M/A time (h)

PGO-Er/Yb:Ag40.3GeO2-59.7PbO0.5Er2O3-3.0Yb2O3-1.0AgNO31200/4201/2
PGO-Eu:Ag40.3GeO2-59.7PbO0.5Eu2O3-3.0AgNO31200/4201/3
BGO-Eu:Au58.4GeO2-41.6Bi2O30.5Eu2O3-3.0Au2O31100/4201/3
BGO-Er:Si58.4GeO2-41.6Bi2O30.5Er2O3-0.2Si nanopowder1100/4201/3
TZO-Er:Ag85.0TeO2-15.0ZnO0.5Tm2O3-2.0AgNO3800/32520/2
TWB-Er:Ag54.5TeO2-22.6WO3-22.7Bi2O31.0Er2O3-2.0AgNO3760/36045/1