Research Article

Mineral Phases and Release Behaviors of As in the Process of Sintering Residues Containing As at High Temperature

Table 3

The As leaching concentration of sintered products at different sintering temperatures.

Sintering temperature (°C)HVEP (mg/L)TCLP (mg/L)

0(1)0.5680.751
10000.9621.444
10500.7031.3
11000.3150.925
12000.0020.0017
13000.0010.0014
13500.0010.0008

The specimen was not sintered at 0°C.