Research Article

Effects of Using Silica Fume and Polycarboxylate-Type Superplasticizer on Physical Properties of Cementitious Grout Mixtures for Semiflexible Pavement Surfacing

Table 3

Selected designs and flexural strength of cementitious grout mixtures.

Grout mixture designPercentage of SP (%)Water/cement ratioFlowability (s) Compressive strength (N/mm2) Flexural strength (N/mm2)
1 day28 days7 days28 days

95% OPC + 5% SF1.50.3018.055.491.76.57.2
95% OPC + 5% SF2.00.3015.057.592.56.79.1
95% OPC + 5% SF2.00.3214.257.191.55.88.3
100% OPC 2.00.3019.359.387.23.86.1