Research Article
Study on Strength and Ultrasonic Velocity of Air-Entrained Concrete and Plain Concrete in Cold Environment
Table 5
The splitting and tensile strength of plain concrete after F-T cycles (MPa).
| W/C | Number of F-T cycles | 0 | 25 | 50 | 75 | 100 |
| 0.55 | Tensile strength | 1.93 | 1.36 | 0.84 | 0.56 | / | Splitting strength | 2.13 | 1.85 | 1.62 | 1.26 | 1.18 |
| 0.5 | Tensile strength | 3.14 | 1.32 | 1.15 | 0.98 | / | Splitting strength | 2.73 | 2.04 | 1.64 | 1.49 | 1.33 |
| 0.45 | Tensile strength | 3.61 | 1.99 | 1.36 | 1.18 | / | Splitting strength | 3.31 | 2.93 | 2.62 | 2.03 | 1.53 |
|
|