Research Article
Obtaining Martensitic Structures during Thixoforming of Hypoeutectic Gray Cast Iron
Table 2
Sequence of tests performed.
| Temperature (°C) | Liquid fraction (%) | Holding time (s) | Cooled sample stuck to platen? | Martensite formed? |
| 1145 | 45 | 0 | No | No |
| 1135 | 30 | 0 | No | No |
| 1130 | 10 | 0 | Yes | Yes | 30 | Yes | Yes | 60 | Yes | Yes | 90 | No | No |
|
|