Durability and Shrinkage Characteristics of Self-Compacting Concretes Containing Recycled Coarse and/or Fine Aggregates
Table 5
Durability tests results of SCCs at 56 days.
| Mix series | Mix code | Charge passed (coulombs) | Gas permeability coefficient () | Sorptivity coefficient (mm/min0.5) | Water penetration depth (mm) |
| Series I | 0.3RCA0RFA0SF0 | 494.3 | 1.446 | 0.0439 | 5 | 0.3RCA0RFA0SF10 | 308.7 | 1.047 | 0.0254 | 4 | 0.43RCA0RFA0SF0 | 685.4 | 1.824 | 0.0458 | 10 | 0.43RCA0RFA0SF10 | 612.0 | 1.304 | 0.0275 | 8 |
| Series II | 0.3RCA100RFA0SF0 | 1574.3 | 2.677 | 0.0538 | 30 | 0.3RCA100RFA0SF10 | 745.6 | 1.987 | 0.0312 | 13 | 0.43RCA100RFA0SF0 | 2323.4 | 3.617 | 0.0647 | 38 | 0.43RCA100RFA0SF10 | 1404.7 | 2.727 | 0.0446 | 25 |
| Series III | 0.3RCA0RFA100SF0 | 1570.7 | 3.466 | 0.0756 | 35 | 0.3RCA0RFA100SF10 | 989.4 | 2.488 | 0.0387 | 22 | 0.43RCA0RFA100SF0 | 2306.9 | 5.015 | 0.0812 | 40 | 0.43RCA0RFA100SF10 | 1618.4 | 3.747 | 0.055 | 31 |
| Series IV | 0.3RCA100RFA100SF0 | 2371.1 | 5.817 | 0.0783 | 38 | 0.3RCA100RFA100SF10 | 1982.9 | 4.716 | 0.057 | 25 | 0.43RCA100RFA100SF0 | 3527.8 | 8.827 | 0.1011 | 55 | 0.43RCA100RFA100SF10 | 2412.6 | 6.618 | 0.0609 | 35 |
|
|