Research Article

Effect of Wood Preservatives on Surface Properties of Coated Wood

Table 2

Average retention and surface roughness results of untreated and treated samples.

PineBeechChestnut
[μm] [μm] [μm]Retention (kg/m3)Retention (kg/m3)Retention (kg/m3)

Untreated (Control) 2.67
(0.94)
27.13
(11.62)
21.82
(8.42)
2.87
(0.90)
32.97
(11.18)
25.31
(6.74)
5.44
(1.12)
82.41
(14.40)
55.31
(14.49)

2% CCA3.25
(0.70)
35.74
(13.33)
27.21
(6.43)
15.67
(0.78)
4.74
(1.38)
42.73
(9.91)
37.39
(8.49)
13.28
(0.66)
6.20
(1.52)
90.54
(17.1)
59.02
(16.1)
10.25
(0.52)

2% Tanalith E 3.28
(0.98)
29.26
(9.15)
24.61
(6.09)
15.39
(0.56)
3.75
(1.32)
38.60
(11.48)
31.39
(6.69)
12.01
(0.45)
5.92
(1.15)
106.05
(19.28)
57.31
(7.89)
10.36
(0.78)

1% Boric acid 2.86
(0.60)
28.41
(7.12)
24.12
(4.75)
6.92
(0.34)
3.45
(0.97)
33.01
(7.69)
29.23
(6.65)
5.77
(0.36)
9.38
(2.73)
106.42
(19.91)
77.37
(22.30)
5.14
(0.28)

Immersol aqua1.92
(0.32)
20.43
(8.17)
16.44
(5.07)
715.96
(37.64)
1.99
(0.55)
19.88
(5.57)
18.27
(4.31)
481.83
(25.96)
7.53
(1.84)
67.92
(8.13)
54.30
(9.48)
377.49
(20.69)

Values in parenthesis are standard deviations.