Specimen numberDiameter/mmHeight/mmNumber of mixing ratiosUniaxial compressive strength/kPaElasticity modulus/kPa

P1146.58102.3268251.931110.083
P1246.16101.1667358.3881754.256
P1346.82103.4866478.8183401.377
P1446.64102.70655100.4074008.291
P2146.38100.5278244.100961.323
P2246.18102.0277352.4781698.07
P2346.58103.0476464.0092629.804
P2446.22102.3875588.6003862.366
P3146.46101.2288237.667830.820
P3246.64102.6687343.9581548.728
P3346.52102.4286453.9352252.316
P3446.50102.4885572.0923480.833
P4146.58101.5498228.542813.918
P4246.56102.8697338.6731311.437
P4346.76102.7296448.1992133.269
P4446.28100.2695558.4872941.296