Frequency2.0 Hz0.05 HzFrequency2.0 Hz0.05 Hz
Cycle [MPa] [MPa]Difference [%]Cycle Difference [%]

131.7333.90%131.633.76.4%
231.5334.50%231.729.86.2%
330.932.44.60%328.327.81.8%
429.431.87.50%425.725.21.9%
529.331.15.80%523.723.31.8%
628.430.56.90%622.121.71.8%
727.829.97.00%720.820.42.0%
827.329.47.10%819.619.22.5%
926.228.89.00%918.518.03.1%
1026.028.69.10%1017.517.03.1%
1125.827.76.90%1116.316.02.1%
1225.227.17.00%1215.015.11.0%
1324.626.36.50%1313.314.36.8%
1423.825.56.70%
1523.224.24.10%
1622.621.64.60%

Total433.7460.95.90% (tot)284.1281.50.92% (tot)