Research Article
The Albedo of Pervious Cement Concrete Linearly Decreases with Porosity
| Number | Sand ratio | w/c ratio | Mix (kg/m³) | Target porosity | Density (kg/m3) | Cement | Aggregate | Sand | WRA | Water |
| 1 | 0.10 | 0.28 | 243.03 | 1518.92 | 151.89 | 2.43 | 124.20 | 0.35 | 1701 | 2 | 0.20 | 0.28 | 245.89 | 1536.79 | 307.36 | 2.46 | 125.66 | 0.30 | 1737 | 3 | 0.30 | 0.28 | 248.81 | 1555.07 | 466.52 | 2.49 | 127.16 | 0.25 | 1812 | 4 | 0.40 | 0.28 | 251.81 | 1573.80 | 629.52 | 2.52 | 128.69 | 0.20 | 1928 |
|
|
The density was tested after the samples were fully cured.
|