Experimental results of combination of Materials A and C.
| Content of Material A/% | Content of Material C/% | Initial setting time/min | Final setting time/min | Compressive strength of one day/MPa | Compressive strength of 28 days/MPa | Compressive strength ratio of 28 days/% |
| 0 | 0 | 195 | 258 | 7.8 | 43.9 | 100 | 55 | 0 | 90 | 162 | 9.1 | 37.8 | 86 | 1 | 69 | 124 | 9.7 | 39.9 | 91 | 1.5 | 59 | 104 | 10.3 | 41.5 | 95 | 2 | 48 | 86 | 11.2 | 42.3 | 96 | 2.5 | 41 | 80 | 11.1 | 42.8 | 97 | 3 | 47 | 85 | 10.8 | 43.1 | 98 |
|
|