Concrete mix properties and strength.
| Design strength grade | C60 | C80 | C100 |
| Water cementitious ratio | 0.30 | 0.26 | 0.24 | Cement (kg/m3) | 350 | 450 | 450 | Coarse aggregate (kg/m3) | 700 | 544 | 510 | Fine aggregate (kg/m3) | 1150 | 1156 | 1190 | Water (kg/m3) | 150 | 156 | 144 | Superplasticizer (kg/m3) | 8 | 12 | 12 | Silica fume (kg/m3) | 0 | 30 | 60 | Fly ash (kg/m3) | 150 | 120 | 90 | Cube compressive strength (MPa) | 79.82 | 87.89 | 109.54 | Axial compressive strength (MPa) | 68.25 | 78.49 | 95.07 | Modulus of elasticity (MPa) | 41675 | 42042 | 42885 |
|
|