Research Article
Influence of Steam Curing Method on the Performance of Concrete Containing a Large Portion of Mineral Admixtures
Table 4
Removal strengths under different curing conditions.
| Samples | Thermostatic temperature/°C | Thermostatic time/h | Removal strength/MPa |
| C | 60 | 9 | 28.7 | F30 | 60 | 11 | 23.7 | 80 | 9 | 35.7 | F40 | 60 | 11 | 17.7 | 80 | 9 | 29.7 | F50 | 60 | 13 | 10.4 | 80 | 11 | 26.8 | B30 | 60 | 11 | 27.8 | 80 | 9 | 31.0 | B40 | 60 | 11 | 32.7 | 80 | 9 | 27.2 | B50 | 60 | 11 | 20.0 | 80 | 9 | 22.6 | B60 | 60 | 11 | 19.4 | 80 | 10 | 27.8 |
|
|