Research Article
Properties of Ready Mixed Acrylic Paste for Exterior Insulation Using Pozzolanic Materials and Atomizing Slag
Table 12
pH and viscosity of the RMAP.
| ā | Plain | P-AS10 | P-AS20 | FM-AS10 | FM-AS20 |
| Unit weight (kg) | 2105 | 2160 | 2210 | 2140 | 2190 | Segregation | Initial | Not detected | Not detected | Not detected | Not detected | Not detected | 6 months | Not detected | Detected | Detected | Not detected | Not detected |
| Viscosity (cP) | Initial | 10,000 | 9,200 | 8,700 | 11,200 | 11,600 | 6 months | 10,500 | 9,300 | 8,750 | 11,500 | 11,300 | Flow (mm) | ā | 160 | 165 | 170 | 170 | 175 |
|
|