Research Article
Investigation of Cement-Emulsified Asphalt in Plastic Concrete
Table 5
Properties of cement-emulsified asphalt concrete under different water-binder ratios.
| Samples | Compressive strength (MPa) | Splitting tensile strength (MPa) | Elastic modulus (GPa) | Tensile strength (MPa) | 14 d | 28 d | 90 d | 14 d | 28 d | 90 d | 14 d | 28 d | 90 d | 28 d | 90 d |
| Xq1 | 6.7 | 9.5 | 15.1 | 0.64 | 0.93 | 1.33 | 2.96 | 4.81 | 10.53 | 0.88 | 1.04 | Xq6 | 5.6 | 8.2 | 13.3 | 0.55 | 0.80 | 1.19 | 2.48 | 3.53 | 5.14 | 0.73 | 0.90 | Xq12 | 4.8 | 7.2 | 10.5 | 0.50 | 0.70 | 1.00 | 1.16 | 3.04 | 4.53 | 0.65 | 0.85 | Xq2 | 4.1 | 5.4 | 7.7 | 0.38 | 0.53 | 0.70 | 1.98 | 2.48 | 3.07 | 0.50 | 0.65 | Xq10 | 3.6 | 5.0 | 6.9 | 0.34 | 0.50 | 0.68 | 1.15 | 2.18 | 3.16 | 0.45 | 0.57 | Xq15 | 3.2 | 4.0 | 5.9 | 0.30 | 0.38 | 0.60 | 0.62 | 1.01 | 1.68 | 0.38 | 0.50 |
|
|