Research Article
Fatigue Performance of SFPSC under Hot-Wet Environments and Cyclic Bending Loads
Table 3
Experimental conditions and results of group E∼G specimens.
| Specimen number | Temperature, T (°C) | Relative humidity, H (%RH) | Stress level, SR=Pmax/Pu | Loading frequency, f (Hz) | Fatigue lives, Nf/cycles |
| E1 | 50 | 80 | 0.60 | 2 | 1678342 | E2 | 1048011 | E3 | 410854 | E4 | 0.65 | 2 | 470951 | E5 | 338499 | E6 | 336204 | E7 | 0.70 | 2 | 249136 | E8 | 0.75 | 2 | 3082 | E9 | 1733 | F1 | 50 | 95 | 0.60 | 2 | >2000000 | F2 | >2000000 | F3 | 0.67 | 2 | 3106 | F4 | 13237 | F5 | 18525 | F6 | 50766 | F7 | 0.72 | 2 | 4266 | F8 | 15037 | F9 | 16241 | F10 | 0.77 | 2 | 223 | F11 | 906 | F12 | 151 | G1 | 35 | 95 | 0.60 | 2 | >2000000 | G2 | 0.70 | >2000000 | G3 | 0.72 | 39535 | G4 | 0.75 | 27171 | G5 | 1549 |
|
|