Grit-blasting, spraying, and remelting process parameters.
| Process | Parameters | Values |
| Grit blasting | Air pressure (MPa) | 0.7 | Blasting distance (mm) | 300 | Blasting angle (°) | 90 |
| Plasma spraying | Voltage (V) | 60 | Current (A) | 500 | Spraying distance (mm) | 150 | Cooling of substrate | Air blow | Gas flow rate (L/min) | Ar(80) | H2(130) | Coating thickness (mm) | 0.80 |
| TIG remelting | Current (A) | 90 | Arc length (mm) | 2 | Argon flow (L·min−1) | 10 | Scanning speed (mm·min−1) | 150 | Step size (mm) | 3 |
|
|