Research Article
[Retracted] Microstructure and Fatigue Properties of 6061 Aluminum Alloy Laser-MIG Hybrid Welding Joint
Table.3
Date of fatigue tests of 6061 BM and welded joints.
| Type | Samples | Maximum stress (MPa) | Stress amplitude (MPa) | Cycles | Fracture location |
| WJ | WJ-1 | 230 | 103.5 | 87186 | Welded zone | WJ | WJ-2 | 220 | 99 | 198378 | Welded zone | WJ | WJ-3 | 210 | 94.5 | 485937 | Welded zone | WJ | WJ-4 | 200 | 90 | 621441 | Welded zone | WJ | WJ-5 | 190 | 85.5 | 834052 | Welded zone | WJ | WJ-6 | 180 | 81 | 1000000 | No broken | BM | BM-1 | 280 | 126 | 388767 | Parallel section | BM | BM-2 | 260 | 117 | 90957 | Parallel section | BM | BM-3 | 240 | 108 | 101975 | Parallel section | BM | BM-4 | 220 | 99 | 232716 | Parallel section | BM | BM-5 | 200 | 90 | 730736 | Parallel section | BM | BM-6 | 180 | 81 | 1000000 | No broken |
|
|