Electrical conductivities and area specific resistances of the prepared samples.

Temperature (°C)σ (Scm−1)ASR (Ω·cm2)
CeZr0CeZr1CeZr2CeZr3CeZr0CeZr1CeZr2CeZr3

2509.5110.4111.9513.520.14860.14280.13650.1295
30010.6712.4514.8617.190.13320.12750.12080.1152
35011.1313.3117.0821.440.12560.12010.11490.1095
40012.2517.4921.7830.790.11920.11320.10740.1025
45015.6222.2632.7442.760.11290.10760.10210.0980