Physical and mechanical parameters of limestone after heat treatment under different heating conditions.

T (°C)ρ (g/cm3) (km/s)UCS (MPa)ε0 (×10-2)Ea (GPa)E50 (GPa)σci (MPa)σci/UCS
MeStMeStMeStMeStMeStMeStMeStMeSt

252.740.0215.350.238121.603.3930.530.00128.841.53820.920.90255.381.1750.460.016
200-V2.740.0123.810.207105.721.1600.590.04725.220.82716.171.60550.221.8100.470.012
200-A2.700.0093.530.24592.663.6350.580.05924.451.45014.461.48540.632.7580.440.013
300-V2.720.0023.210.13291.272.1140.610.01321.580.62912.710.76440.472.6300.440.019
300-A2.710.0102.800.07678.464.8790.640.00319.500.9059.971.02533.973.9390.430.023
450-V2.700.0272.370.02188.988.3090.860.02817.040.9768.470.64336.542.8360.410.007
450-A2.680.0162.090.06274.432.5390.870.04113.090.6657.110.26228.833.2600.390.057
600-V2.660.0201.910.05976.763.2881.000.01212.871.5066.490.11330.012.1350.390.045
600-A2.660.0331.710.34263.180.3541.050.0439.791.1174.770.27621.791.1460.340.016
750-V2.640.0181.760.23865.665.4801.230.0458.680.0714.150.25524.122.2910.370.004
750-A2.600.0361.420.14653.891.4991.280.0827.060.4953.290.21217.321.7040.320.041
900-V2.570.0101.530.02535.892.2421.330.0334.390.9052.170.00711.781.4140.330.060
900-A2.520.0251.320.09530.811.7961.490.0282.500.0072.050.1349.710.5520.320.000