Preparation and Characterization of High Modulus Agent Modified Asphalt and Its High Modulus Mixture
Table 3
Technical indexes of SBS asphalt.
| Indicators | Unit | Standard index | Test values | Standard |
| Penetration (25°C, 100g, 5s) | 0.1 | 60–80 | 71.7 | T0604 | Softening point | °C | ≥55 | 72 | T0606 | Ductility (5 cm/min, 15°C) | Cm | ≥30 | 39 | T0605 | After the thin-film oven test (TFOT) | Loss on heating | %Wt. | ≤±1.0 | −0.019 | T0609 | Retained penetration after TFOT | % | ≥60 | 84 | Retained ductility after TFOT | Cm | ≥20 | 32 |
|
|