Typical ranges of constituent materials for high early strength concrete [51, 106110].

Mix characteristic4–6 hours concrete6–8 hours concrete12–16 hours concrete20–24 hour concrete

Cement typeNormal or high early strengthNormal or high early strength or blendedNormal or high early strength or blendedNormal or high early strength or blended
Cement content385–565 kg/m3385–565 kg/m3420–500400–475 kg/m3
W/c ratio0.32–0.400.36–0.400.32–0.460.40–0.47
AcceleratorYesYesNone to yesNone to yes