Research Article
Moisture Stability of Hard Sandstone Asphalt Mixture Based on APT with MMLS3
Table 4
Technical properties of SBS modified asphalt.
| Properties | Unit | Technical requirements | Results |
| Penetration depth at 25°C, 100 g, 5 s | 0.1 mm | 40–60 | 50 | Penetration index | — | ≥0 | 1.152 | Softening point (ring and ball method) | °C | ≥60 | 85.0 | Ductility at 5 cm/min, 5°C | cm | ≥20 | 39 | Specific relative density at 15°C | — | — | 1.060 | Kinematic viscosity at 135°C | Pa·s | ≤3 | 1.2 | Flash point temperature | °C | ≥230 | 303 | Solubility in trichloroethylene | % | ≥99 | 99.54 | Elasticity recovery at 25°C | % | ≥75 | 81 | Rolling thin-film oven test at 163°C | Weight change | % | ±1.0 | −0.105 | Retained penetration | % | ≥65 | 67 | Ductility at 5°C | cm | ≥15 | 19 |
|
|