Results of experiments sorted by sintering factors for mean microhardness HV and signal-to-noise.
| Experimental run | Sintering factors | Responses | Sintering temperature | Sintering pressure | Sintering time | Mean MH | Mean signal to noise ratio | (°C) | (MPa) | (min) | (HV) | (dB) |
| 1 | 500 | 35 | 15 | 51.41 | 34.2140 | 2 | 500 | 45 | 20 | 47.01 | 33.4421 | 3 | 500 | 55 | 25 | 50.41 | 34.0487 | 4 | 550 | 35 | 20 | 54.21 | 34.6801 | 5 | 550 | 45 | 25 | 53.21 | 34.5183 | 6 | 550 | 55 | 15 | 58.61 | 35.3581 | 7 | 600 | 35 | 25 | 49.01 | 33.8040 | 8 | 600 | 45 | 15 | 50.61 | 34.0831 | 9 | 600 | 55 | 20 | 50.01 | 33.9795 |
|
|