Research Article

Optimization of Wear Process Parameters of Al6061-Zircon Composites Using Taguchi Method

Table 5

L 27 orthogonal array with wear.

Sl. No.LoadSpeedSlidingPercentage of reinforcementWear in microns

110200500685
2102001000979
31020015001272
410400500994
51040010001288
6104001500682
71060050012105
81060010006108
91060015009112
1020200500667
11202001000964
122020015001256
1320400500980
142040010001274
15204001500667
16206005001286
17206001000689
18206001500992
1930200500655
20302001000951
213020015001249
2230400500967
233040010001261
24304001500656
25306005001277
26306001000673
27306001500970