Research Article
[Retracted] Comparison of Microstructure and Mechanical Properties of A356/SiC Metal Matrix Composites Produced by Two Different Melting Routes
Table 11
Improved toughness of A356/SiC MMC by electromagnetic stir casting process.
|
A356/SiC MMC |
Sample number | Electromagnetic stir casting samples (ESCS) | Mechanical stir casting samples (MSCS) |
Improved toughness (joule) | Toughness (joule) | Variation (joule) | Average toughness (joule) | Toughness (joule) | Variation (joule) | Average toughness (joule) |
| 100% A356 + 0% SiC | 1 | 6.5 |
0.5 |
6.33 | 6 |
0.5 |
6.16 |
2.68% | 2 | 6.5 | 6.5 | 3 | 6 | 6 |
| 95% A356 + 5% SiC | 1 | 7.5 |
1 |
8 | 7.5 |
1.5 |
7.33 |
8.37% | 2 | 8 | 8 | 3 | 8.5 | 6.5 |
| 90% A356 + 10% SiC | 1 | 11 |
3.5 |
11.5 | 7 |
5 |
10.16 |
11.65% | 2 | 10 | 12 | 3 | 13.5 | 11.5 |
| 85% A356 + 15% SiC | 1 | 15 |
2.5 |
13.5 | 13 |
8 |
12.33 |
8.66% | 2 | 13 | 8 | 3 | 12.5 | 16 |
|
|