Research Article
Performance of Sprayed Fiber Reinforced Polymer Strengthened Timber Beams
Table 2
Summary of results: boracol treated.
| | Ultimate load (kN) | Ultimate displacement (mm) | Energy absorbed (kJ) | Load % increase over A | Energy absorbed % increase over A | FRP rupture |
| Beam A | 184.7 | 20.1 | 2.4 | — | — | — | Beam B | 210.1 | 22 | 2.1 | 13.8% | −12.5% | No | Beam C* | 181.4 | — | — | −1.8% | — | No | Beam D | 215.2 | 31.6 | 4.8 | 16.5% | 100.0% | Yes | Beam E | 215.4 | 30.1 | 4.4 | 16.6% | 83.3% | Yes |
|
|
*Due to a data acquisition failure, displacements, and strain gauge readings from Beam C were not properly recorded.
|