Table 7

Test scheme and compressive strength index results.

Test ID Compressive strength (MPa)
Fine aggregate : coarse aggregatesBarite sand : quartz sandAnhydrous sodium silicate : aggregatesAnhydrous sodium silicate : sodium fluorosilicate12345

10.29490.29840.21880.19950.29121.30280.2606
20.57850.58320.70680.57230.65113.09180.6184
32.53662.74292.48552.60602.739913.11102.6222
44.14033.67294.78844.08764.545621.23484.2470
50.54080.48130.60270.42280.55292.60050.5201
60.12280.15490.17060.20800.15920.81550.1631
71.76781.51831.51021.41431.91268.12321.6246
80.99761.01441.07130.84840.95944.89120.9782
91.32421.19961.91821.98212.00068.42471.6849
102.31291.62851.88882.48491.38789.70291.9406
110.26540.18760.21820.25080.21501.13700.2274
120.20490.13920.22930.18640.24271.00260.2005
130.84330.82100.79650.86150.82514.14750.8295
140.39360.38800.37820.34160.38351.88490.3770
150.32920.47200.50580.37800.44332.12840.4257
160.25330.18710.22650.22560.23691.12940.2259

38.740416.47554.384712.3135;
16.430415.49518.823313.2675
20.267224.499628.311826.5438
9.290228.25843.208432.6034