Research Article
Fresh and Mechanical Properties of Self-Compacting Rubber Lightweight Aggregate Concrete and Corresponding Mortar
Table 4
Test results of fresh properties of SCRLC.
| Type of concrete | SF (mm) | T500 (s) | Tv (s) | T400 (s) | h2/h1 (s) | Δh (mm) | SR (%) |
| SCLC | 785 | 5.6 | 14.7 | 7.3 | 0.98 | 3 | 10.8 | SCRLC10 | 770 | 5.8 | 15.6 | 7.5 | 0.97 | 4 | 9.7 | SCRLC20 | 740 | 6.2 | 16.9 | 8.1 | 0.94 | 7 | 8.3 | SCRLC30 | 710 | 6.7 | 18.5 | 8.5 | 0.92 | 9 | 7.5 | SCRLC40 | 650 | 7.9 | 21.6 | 9.3 | 0.87 | 14 | 4.9 | SCRLC50 | 580 | 9.4 | 24.3 | 10.9 | 0.82 | 18 | 3.2 |
|
|