Hybrid Modification of Stone Mastic Asphalt with Cellulose and Basalt Fiber
Table 2
Mass loss of cellulose and basal fiber.
| Fiber | Test procedure | Mass before heat (g) | Mass after heat (g) | Mass loss (%) | Visual change of fiber |
| Basalt fiber | 165°C, 2 h | 1.0180 | 1.0155 | 0.246 | No change. | 165°C, 5 h | 1.0442 | 1.0416 | 0.249 | 200°C, 2 h | 1.0334 | 1.0269 | 0.629 | 200°C, 5 h | 1.0118 | 1.0053 | 0.642 | Cellulose fiber | 165°C, 2 h | 1.0120 | 0.9624 | 4.901 | Fiber curl, and color of surface becomes darker. | 165°C, 5 h | 1.0563 | 0.9829 | 6.949 | 200°C, 2 h | 1.0248 | 0.9278 | 9.465 | 200°C, 5 h | 1.0007 | 0.8809 | 11.972 |
|
|