OAC and volumetric properties of SMA with different fiber combinations.

Cellulose : basaltOAC (%) (asphalt-aggregate ratio)VV (%)VMA (%)VFA (%)

0 : 45.93.616.579.4
1 : 36.03.816.677.1
2 : 26.13.917.077.6
3 : 16.13.216.780.8
4 : 06.23.417.279.0
0 : 05.44.216.075.3