Tensile strength of CSES and CSI solder joints (before and after corrosion).

Solder materialCSES (before corrosion)CSI (before corrosion)CSES (after corrosion)CSI (after corrosion)
Tensile strength (MPa)Std devi.Tensile strength (MPa)Std devi.Tensile strength (MPa)Std devi.Tensile strength (MPa)Std devi.

SAC30546.8941.152345.1821.164339.8951.452338.9931.1723
SACX030735.2071.194334.1542.194328.8611.294327.9231.2943
99C31.9041.233330.1891.533325.2431.533323.3781.2633