Research Article
Experimental Study on Dynamic Mechanical Properties of Coal Gangue Concrete
Table 5
Compressive strength of concrete after conversion.
| Group | Numbering | Compressive strength (MPa) | Compressive strength growth rate | 3 days | 7 days | 28 days | 60 days | 90 days | 3–7 days | 7–28 days | 28–60 days | 60–90 days |
| C30 | NAC | 26.45 | 31.50 | 39.94 | 43.42 | 46.42 | 0.191 | 0.268 | 0.087 | 0.069 | N-SFC | 24.34 | 31.08 | 44.67 | 49.10 | 52.94 | 0.277 | 0.437 | 0.099 | 0.078 | N-SAC | 23.30 | 31.12 | 39.07 | 42.47 | 43.91 | 0.336 | 0.255 | 0.087 | 0.034 | N-SC | 22.39 | 31.35 | 41.83 | 45.67 | 47.43 | 0.400 | 0.334 | 0.092 | 0.039 |
| C40 | NAC | 36.14 | 41.87 | 48.62 | 53.04 | 55.92 | 0.159 | 0.161 | 0.091 | 0.053 | N-SFC | 31.29 | 40.32 | 54.42 | 59.42 | 60.96 | 0.289 | 0.35 | 0.092 | 0.053 | N-SAC | 29.46 | 41.74 | 47.34 | 50.11 | 52.50 | 0.417 | 0.134 | 0.059 | 0.034 | N-SC | 27.89 | 42.00 | 49.79 | 53.65 | 55.69 | 0.506 | 0.185 | 0.078 | 0.038 |
|
|